Lost-foam (Full-mold) Pouring Parameters

消失模实型浇注参数与白模密度

type:tutorial · level:intermediate · material:copper · material:brass · variant:lost-foam · scale:industrial · scale:sculpture · equipment:furnace · equipment:hand-tools · stage:patternmaking · stage:pouring

标签:消失模, 泡沫模样, 实型铸造, EPS

消失模用 EPS/STMMA 泡沫模样埋入干砂振动紧实后直接浇注,铜液前沿气化白模并维持负压(–0.03~–0.05 MPa)充型。关键参数:白模密度 18–25 g/L(过高积碳、过低变形),浇温比砂型高 30–50 ℃(黄铜 1000–1050 ℃),涂层透气性决定充型速度。适合艺术雕塑批量复制;表面会保留细小珠粒橘皮纹,需抛光或有意保留作肌理。

Lost-foam pours directly into dry sand around an EPS/STMMA pattern under vacuum (–0.03 to –0.05 MPa) as the metal front vaporizes the foam. Key parameters: pattern density 18–25 g/L (higher causes carbon deposits, lower distorts), pouring temperature 30–50 °C above green sand (brass at 1000–1050 °C), and coating permeability controls fill rate. Great for art reproduction; expect fine bead orange-peel texture—polish it out or keep it as a designed surface. ---