Laser-Engraved Mould Texture Recipe

激光雕刻模具纹理配方

type:recipe · level:advanced · material:bronze · scale:industrial · stage:patternmaking

标签:激光雕刻,模具纹理,光纤激光,重铸层,粘模

以 30–60 W 光纤激光在模具钢或青铜模面直接雕刻纹理,扫描速度 800–1200 mm/s、单道功率 60%–80%,深度按道数累积(每道约 0.02–0.03 mm)。雕刻后用 800 目油石轻研去除熔渣重铸层,再以 5% 硝酸酒精轻蚀 10 秒统一表面光泽,可显著减少铸件粘模。

Engrave textures directly into tool-steel or bronze mould faces with a 30–60 W fibre laser at 800–1200 mm/s and 60%–80% single-pass power; depth accumulates about 0.02–0.03 mm per pass. After engraving, remove the recast layer with an 800-grit stone, then etch 10 s in 5% nitric-alcohol to unify lustre—this markedly reduces casting sticking. ---